The success or failure of CPC molds lies in the sealing flatness and exhaust groove depth, both measured in 0.01 millimeters.

  • Vistas: ...
  • Tempo de liberação: 2026-11-16

The success or failure of CPC molds lies in the sealing flatness and exhaust groove depth, both measured in 0.01 millimeters.

1、 Flatness of sealing surface

 

When the flatness exceeds 0.05 millimeters, the back pressure is often not established enough, and the porosity rises to over 2%.

The sealing surface needs to be finely ground and the roughness should be controlled within Ra0.8.

2、 Sealing structure and redundancy

A single set of molds usually has two redundant seals, and the material needs to withstand temperatures above 300 degrees Celsius.

The compression amount of the sealing ring should be set at 15% to 20%, as excessive compression can cause permanent deformation.

Sealing failure often occurs when the mold is closed under unbalanced load, and the parallelism of the press needs to be checked.

3、 Exhaust groove accuracy

The depth of the exhaust groove is taken as 0.10 to 0.15 millimeters, with a tolerance controlled within plus or minus 0.01 millimeters.

If the groove depth exceeds 0.18 millimeters, aluminum will run away, and if it is below 0.08 millimeters, there will be insufficient exhaust.

The total exhaust area shall be configured to be no less than 120 square millimeters per meter of the cavity circumference.

4、 Pressure establishment and leak detection

The back pressure is usually set at 0.8 to 1.2 megapascals, and the establishment time is controlled within 5 seconds.

It is recommended to perform pressure testing before each mold closing, and if the pressure drop exceeds 5%, it will be judged as a leak.

Xinfeng has installed a leak detection interface on the CPC mold to facilitate quick judgment on the production line.

5、 Verification and maintenance

The first CT or slice should be done, and the porosity should be below 0.8% to meet the standard.

The sealing ring is recommended to be replaced every 3000 to 5000 molds and should not be used beyond the expiration date.

Industry data shows that after the implementation of the leak detection system, the CPC scrap rate can be reduced by about 30%.

Conclusion and Outlook

The accuracy of CPC is not in the cavity, but in the small scale of sealing and exhaust.

Only by controlling the flatness and groove depth can the pressure be stably established.

Extension: Three maintenance actions for CPC molds

Action 1: Clean the sealing surface before each mold closing, as oil stains can distort the compression amount.

Action 2: Measure the size of the sealing ring every 3000 cycles, and replace it if the compression is less than 15%.

Action 3: Check the depth of the exhaust groove for each batch, and if it exceeds 0.18 millimeters, it needs to be repaired.

The three actions form a cycle, and the pressure is only stable when it is established.

Comparing maintenance records with pressure curves makes it easier to locate leaks.

Xinfeng attached a maintenance schedule and leak detection record template when delivering CPC molds.

Addendum: Four daily actions of sealing and exhaust

The sealing surface needs to be cleaned before each mold closing, as oil stains can cause the actual compression to deviate from the design value.

It is recommended to replace the sealing ring according to the mold number, as the probability of leakage increases significantly after expiration.

If the leak detection pressure drop exceeds 5%, it is judged as a leak and needs to be stopped for processing instead of continuing production.

The depth of the exhaust groove needs to be measured after processing, and if the deviation exceeds 0.02 millimeters, it should be repaired.

Addendum 2: Three acceptance criteria for CPC molds

The porosity of the first piece should be less than 0.8%, and the testing method and sampling location should be indicated.

The flatness of the sealing surface and the depth of the exhaust groove need to be measured and recorded, and cannot be judged solely by visual inspection.

The leak detection pressure drop should be controlled within 5%, and exceeding the standard is considered as unqualified.

FAQ

What is the requirement for the flatness of the sealing surface? It needs to reach 0.02 millimeters.

What will happen if it exceeds 0.05 millimeters? Insufficient pressure establishment leads to an increase in porosity.

How many seals are needed? Usually there are two redundancies.

What is the compression amount of the sealing ring? 15% to 20%.

What is the depth of the exhaust groove? 0.10 to 0.15 millimeters, with a tolerance of plus or minus 0.01 millimeters.

What is the back pressure? 0.8 to 1.2 megapascals.

How long does it take to replace the sealing ring? Suggest 3000 to 5000 cycles.
Aluminum alloy casting blank allowance: choice between 1.5mm and 3mm

Excessive blank allowance increases working hours, while insufficient allowance exposes black skin. Setting according to location and tolerance zones is more reasonable.

1、 Benchmark algorithm for margin

The blank allowance of castings is usually taken as 1.5 to 2.5 millimeters, with the upper limit for large pieces and the lower limit for small pieces.

For every 1 millimeter increase in margin, machining hours increase by approximately 10% to 15%.

When the margin is less than 1 millimeter, dimensional fluctuations can easily lead to local unprocessed parts.

2、 Partition by location

Take a margin of 1.5 to 2 millimeters for the critical installation surface to ensure precise machining with just one cut.

There is no allowance for non machined surfaces, only a 0.5mm cleaning amount is retained.

The allowance in the thick walled area can be 0.5 millimeters more than that in the thin walled area to offset the shrinkage difference.

3、 Corresponding to the mold cavity

The cavity size is designed according to the nominal size of the casting with allowance, and the shrinkage rate is compensated by 0.6% to 1.0%.

The shrinkage rate is taken incorrectly by 0.2 percentage points, and the size deviation of large items can exceed 1 millimeter.

The mold cavity should be consistent with the machining reference to avoid secondary clamping deviation.

4、 Machining and Fixtures

Uneven margin can cause the blade to vibrate and the surface roughness to deteriorate by about one level.

The positioning surface of the fixture should be consistent with the mold reference, and the positioning error should be controlled within 0.05 millimeters.

It is recommended to roughen the thin-walled parts first and then refine them, with stress relief arranged in the middle.

5、 Verification and adjustment

Measure the residual distribution of the first piece and record it point by point. If the deviation exceeds 0.5 millimeters, the mold needs to be repaired.

During the batch stage, the critical surface allowance is reviewed every 500 pieces.

Industry practice shows that after optimizing the margin partition, machining hours have decreased by about 12%.

Conclusion and Outlook

The margin is not necessarily the thicker, the safer it is, but it should match the tolerance and process.

Implement partition setting, shrinkage compensation, and benchmark unification to reduce both exposed black skin and out of tolerance.

Extension: Three checks for margin design

Check one: whether the margin covers the upper limit of shrinkage deviation, and large items often need to reserve more than 0.8 millimeters.

Verification 2: The number of machining clamping times, secondary clamping will introduce a benchmark error of 0.05 millimeters.

Check three: Do we need to add extra allowance separately for the thin-walled area? The deformation direction of the thin-walled area is opposite to that of the thick wall.

Three items are missing in the verification, and the probability of the first item showing black skin has significantly increased.

During the mold design phase, Xinfeng attached a distribution diagram of the remaining allowance to facilitate alignment between the customer and the machining party.

The surplus diagram is issued synchronously with the process card, making it easier to trace deviations during the batch stage.

Addendum: Four Methods for Surplus Confirmation

The margin setting should refer to the historical data of the same family of parts, and the deviation can usually converge to within 0.3 millimeters.

The first piece allowance measurement needs to be carried out after heat treatment, and the measurement before heat treatment may be distorted due to deformation.

The margin diagram should indicate the machined and non machined surfaces to avoid misjudgment by the machining side.

Recheck the critical surface allowance every 500 pieces in the batch to clarify the drift trend.

Addendum 2: Coordination between Surplus and Process

Leave a precision machining allowance of 0.5 millimeters for rough machining, and casting defects may be exposed when the allowance is insufficient.

Arranging the stress relief process after rough machining can reduce subsequent deformation by about 0.2 millimeters.

FAQ

How much margin is appropriate? Usually take 1.5 to 2.5 millimeters.

How many working hours does it take to increase the margin by 1 millimeter? About 10% to 15%.

What is the shrinkage rate? 0.6% to 1.0%, adjusted according to the brand.

What are the consequences of not having enough margin? Make the knife and roughness worse.

How much is the fixture positioning error controlled? Within 0.05 millimeters.

Do we need to measure the margin for the first piece? Need to record deviations point by point.

How many hours can surplus optimization save? About 12%.

Aluminum alloy casting mold assembly and mold debugging: four inspections before the first test

Sítio Web Deste artigo: https://pt.zj-xinfeng.com/case/1511.html

Get a Custom Product Proposal Online

Please fill out the form below to receive this for free.

Global Hotline:

+86-15356852630,13967513266

Moldes para fundição por baixa pressão (LPDC) 
Moldes para fundição por gravidade 
Moldes para fundição por contrapressão (CPC) 
Moldes para fundição de peças estruturais
Molde para fundição de cubos de roda de motocicleta
Molde para fundição por pressão diferencial de cubos de roda
Molde para fundição por gravidade de cubos de roda
Molde para fundição por baixa pressão de cubos de roda

MOLDES PARA JANTES AUTOMÓVEIS 
PEÇAS ESTRUTURAIS AUTOMÓVEIS 
OUTROS COMPONENTES DE FUNDIDOS DE ALUMÍNIO

NOTÍCIAS DA EMPRESA
NOTÍCIAS DO SETOR
BLOG TÉCNICO
PERGUNTAS FREQUENTES

PERFIL DA EMPRESA
ESTRUTURA ORGANIZACIONAL
HISTÓRICO DE DESENVOLVIMENTO
PROPRIEDADE INTELECTUAL
ESPÍRITO DE EQUIPA PARCEIRO

Copyright © Zhejiang Xinfeng Machinery Co., Ltd. All Rights Reserved.