LPDC riser and pressurization curve: two parameters for smooth filling

  • Vistas: ...
  • Tempo de liberação: 2026-11-16

LPDC riser and pressurization curve: two parameters for smooth filling

The charging quality of LPDC is determined by the liquid lifting speed and pressure gradient, with smoothness being superior to speed.

1、 Liquid lifting stage

The liquid lifting speed is often set at 0.2 to 0.5 meters per second, and too fast can cause liquid level impact and gas entrainment.

The lifting time is calculated in reverse according to the lifting height and speed, usually 3 to 6 seconds.

The diameter of the riser should match the weight of the casting, as being too thin can cause excessive pressure drop.

2、 Filling stage

It is recommended to control the filling pressure gradient at 0.05 megapascals per second to avoid liquid level turbulence.

The filling time is estimated to be 0.02 to 0.03 seconds per millimeter of wall thickness.

Thin walled parts should be filled quickly, while thick walled parts should be filled slowly to prevent cold insulation and gas entrapment.

3、 Pressure retention and shrinkage compensation

The holding pressure is usually set at 0.6 to 1.0 bar, with the upper limit for safety components.

The holding time is set at 3 to 4 seconds per millimeter of wall thickness, and insufficient time will result in concentrated shrinkage.

After the pressure holding is completed, the pressure should be slowly released to avoid the casting being sucked back.

4、 Maintenance of liquid lifting tube

The lifting tube needs to be preheated to above 600 degrees Celsius, as the cold tube can cause aluminum liquid to solidify and block.

If the thickness of slag deposition on the pipe wall exceeds 2 millimeters, it should be replaced in a timely manner.

Aging of the sealing ring can cause pressure leakage, it is recommended to check every 5000 molds.

5、 Verification and recording

Suggest recording the liquid rise time, filling pressure, and holding pressure curve for each batch.

When the curve deviation exceeds 10%, the sealing and pipe diameter should be rechecked.

Xinfeng provides a recommended pressure curve parameter table when delivering LPDC molds.

Conclusion and Outlook

The smooth charging of LPDC relies on slow rise of liquid and gradual pressurization.

The three parameters of speed, gradient, and holding pressure are fixed, and porosity and shrinkage are controlled simultaneously.

Extension: Three coordination points on the LPDC device side

The liquid level fluctuation of the insulation furnace exceeds 50 millimeters, and the height of the liquid rise changes accordingly, requiring liquid level monitoring.

If the pressure fluctuation of compressed air exceeds 0.05 megapascals, the pressure holding effect will be significantly reduced.

The temperature of the mold and the temperature of the aluminum liquid need to be recorded synchronously, and it cannot be determined by looking at one item alone.

Only when the three coordination points are stable can the curve parameters be meaningful.

Xinfeng provides an equipment parameter checklist upon delivery for customers to check item by item.

By coordinating with shift based inspections, curve drift can be detected in advance.

Addendum: Five maintenance items for the pressurization system

The diameter of the liquid lifting tube is matched according to the weight of the casting, and being too thin will prolong the liquid lifting time by about 30%.

Every time the liquid lifting pipe is replaced, the liquid lifting speed needs to be recalibrated, and the difference in pipe diameter will change the actual flow rate.

The pressure relief speed after the pressure holding is controlled within 0.02 megapascals per second.

When the pressure curve is abnormal, check the seal first and then check the gas source. Reversing the order can easily lead to misjudgment.

Calibrate the pressure sensor every 5000 cycles, and any reading deviation may cause batch misjudgment.

Addendum 2: Three references for LPDC parameter setting

Thin walled parts are designed for fast charging and slow protection, while thick walled parts are designed for slow charging and long protection, with settings based on wall thickness.

It is recommended to record three curves for the first article, which will facilitate subsequent comparison and adjustment.

The parameter fine-tuning range should be controlled within 10%, and significant adjustments can easily introduce new defects.

FAQ

What is the liquid lifting speed? 0.2 to 0.5 meters per second.

How long does it usually take to raise the liquid? Usually 3 to 6 seconds.

What is the filling pressure gradient? Not exceeding 0.05 megapascals per second.

What is the holding pressure? 0.6 to 1.0 bar.

How to calculate the holding time? Wall thickness every millimeter for 3 to 4 seconds.

Do I need to preheat the riser? Preheat to above 600 degrees Celsius.

How long does it take to check the sealing ring? Suggest every 5000 cycles.

CPC reverse pressure casting mold sealing and exhaust accuracy: a difference of two 0.02mm

Sítio Web Deste artigo: https://pt.zj-xinfeng.com/case/1510.html

Get a Custom Product Proposal Online

Please fill out the form below to receive this for free.

Global Hotline:

+86-15356852630,13967513266

Moldes para fundição por baixa pressão (LPDC) 
Moldes para fundição por gravidade 
Moldes para fundição por contrapressão (CPC) 
Moldes para fundição de peças estruturais
Molde para fundição de cubos de roda de motocicleta
Molde para fundição por pressão diferencial de cubos de roda
Molde para fundição por gravidade de cubos de roda
Molde para fundição por baixa pressão de cubos de roda

MOLDES PARA JANTES AUTOMÓVEIS 
PEÇAS ESTRUTURAIS AUTOMÓVEIS 
OUTROS COMPONENTES DE FUNDIDOS DE ALUMÍNIO

NOTÍCIAS DA EMPRESA
NOTÍCIAS DO SETOR
BLOG TÉCNICO
PERGUNTAS FREQUENTES

PERFIL DA EMPRESA
ESTRUTURA ORGANIZACIONAL
HISTÓRICO DE DESENVOLVIMENTO
PROPRIEDADE INTELECTUAL
ESPÍRITO DE EQUIPA PARCEIRO

Copyright © Zhejiang Xinfeng Machinery Co., Ltd. All Rights Reserved.