The key factors in the design of gravity casting runners are cross-sectional area ratio, process balance, and slag blocking structure.
1、 Sectional area ratio
The ratio of the area of the sprue, runner, and sprue is often taken as 1:1.6 to 2.0, forming a sequential filling pattern.
Inverted proportions can cause disordered filling and curling, resulting in an increase of about 20% in porosity.
The total area of the sprue is calculated by reversing the weight of the casting and the filling time, usually taking 8 to 12 square centimeters per kilogram.
2、 Process balance
When using multiple sprues, the difference between the distal and proximal processes should be controlled within 15%.
The process difference is too large, the remote end is prone to cold isolation, and the near end is prone to overheating.
By adjusting the width and position of the sprue, the process difference can be reduced to within 10%.
3、 Slag blocking and filtration
Setting up slag blocking bags or filter screens in the horizontal pouring channel can reduce oxidation inclusions by about 30%.
The aperture of the filter screen is often set at 10 to 20 holes per inch, and being too dense will reduce the filling speed.
The design of the pouring cup should avoid turbulence and control the liquid level drop within 50 millimeters.
4、 Pouring speed and temperature
The pouring speed of gravity casting is usually controlled at a filling height of 50 to 80 millimeters per second.
The pouring temperature is set at 700 to 720 degrees Celsius, with the lower limit for thin-walled components.
When the temperature and speed do not match, the cold insulation and sand adhesion increase simultaneously.
5、 Verification method
First piece slicing or X-ray inspection for density near and far from the sprue.
The design of the sprue combined with CAE can reduce the need for about one trial mold.
Industry practice shows that after optimizing the proportion and slag blocking, the yield of gravity parts has increased by about 12 percentage points.
Conclusion and Outlook
Gravity gating relies on proportional control of flow state and process control of temperature.
The proportion, process, and slag blocking are determined, and the air holes and cold insulation decrease simultaneously.
Extension: Three Processing Requirements for the Pouring System
The roughness of the inner wall of the sprue should be controlled within Ra12.5, as excessive roughness will increase flow resistance.
The rounded corner at the connection between the sprue and the mold cavity should not be less than 3 millimeters to avoid local overheating.
The disassembly and assembly structure of the pouring block should be easy to clean, as residual paint can affect the flow state.
The three processing requirements are often overlooked, but they directly affect the defect rate.
The pouring system can be made into detachable inserts, which can reduce maintenance time by about half.
The processing requirements are written in the drawing annotations, and the supplier's execution is more accurate.
Addendum: Five processing details of the sprue system
It is recommended to use detachable inserts for the pouring system, which can reduce cleaning and replacement time by about half.
The thickness of the sprue is often taken as 0.6 to 0.8 times the wall thickness of the casting, and excessive thickness can prolong the solidification time.
A buffer bag is installed at the bottom of the sprue, which can reduce the impact of air entrainment by about 20%.
Preheat the sprue to above 200 degrees Celsius before pouring, and the probability of first piece cold insulation will significantly decrease.
Inspect the coating on the inner wall of the sprue in each batch, as detachment can contaminate the aluminum liquid and introduce inclusions.
Addendum 2: Three on-site controls for gravity gating
The pouring temperature and runner preheating need to be synchronized, and it is difficult to stabilize the flow state with a single control.
Check whether the inner gate is stuck with aluminum in each batch, as sticking aluminum will change the actual cross-sectional area.
It is recommended to synchronize the cleaning cycle of the sprue with the cleaning chamber, as residual aluminum may introduce inclusions.
FAQ
What is the cross-sectional area ratio? Commonly used ratio is 1:1.6 to 2.0.
What will happen if the proportion is reversed? Irregular filling, with an increase of about 20% in porosity.
How to calculate the area of the sprue? Take 8 to 12 square centimeters per kilogram of casting.
How much is the difference in process control? Suggest within 15%.
What is the aperture of the filter screen? 10 to 20 holes per inch.
How to control the pouring speed? The filling height is 50 to 80 millimeters per second.
How many trial molding sessions can be saved? Cooperate with CAE to save once.
Moldes para fundição por baixa pressão (LPDC)
Moldes para fundição por gravidade
Moldes para fundição por contrapressão (CPC)
Moldes para fundição de peças estruturais
Molde para fundição de cubos de roda de motocicleta
Molde para fundição por pressão diferencial de cubos de roda
Molde para fundição por gravidade de cubos de roda
Molde para fundição por baixa pressão de cubos de roda
MOLDES PARA JANTES AUTOMÓVEIS
PEÇAS ESTRUTURAIS AUTOMÓVEIS
OUTROS COMPONENTES DE FUNDIDOS DE ALUMÍNIO
PERFIL DA EMPRESA
ESTRUTURA ORGANIZACIONAL
HISTÓRICO DE DESENVOLVIMENTO
PROPRIEDADE INTELECTUAL
ESPÍRITO DE EQUIPA PARCEIRO
Copyright © Zhejiang Xinfeng Machinery Co., Ltd. All Rights Reserved.