The hot spots at the root of the spokes are caused by local hot spots and insufficient cooling. The countermeasures are point cooling, structure and rhythm.
1、 Formation of hot spots
The wall thickness at the junction of the spokes and the wheel rim is concentrated, and the solidification lags behind. The mold temperature is often 30 degrees Celsius higher than the surrounding area.
The hardness of the hot spot area is often 10 to 15HB lower, and subsequent machining is prone to tool failure.
When the hot spot is not controlled, the probability of shrinkage in this area increases by about 20%.
2、 Cooling and inlay
Adding a cooling point at the base of the spoke can reduce the local temperature by about 25 degrees Celsius.
It is recommended to use copper alloy with a thermal conductivity higher than 80 watts per meter Kelvin for the cooling insert material.
The timing of starting the cold switch should be synchronized with the end of the charging process, as starting it in advance can cause cold isolation.
3、 Transition between structure and wall thickness
It is recommended that the rounded corner at the root of the spoke be no less than 8 millimeters to avoid stress concentration.
The transition length of wall thickness should be 3 to 5 times the difference in wall thickness to reduce abrupt changes.
After a smooth transition in structure, the hot spot area can be reduced by about 30%.
4、 Rhythm and Spraying
A fluctuation of more than 15% in a single beat will disrupt the thermal balance and cause the hot spot to expand.
The spraying amount in the hot spot area should be less than that in the thin-walled area to avoid local undercooling.
The temperature difference of the mold surface is controlled within plus or minus 5 degrees Celsius, and the influence of hot spots is significantly reduced.
5、 Verification and judgment
Confirm the location of the hot spot and temperature peak using infrared thermography, with a grid spacing of 50 millimeters.
When the temperature difference in the hot spot area exceeds 10 degrees Celsius, the cooling point should be rechecked.
Xinfeng arranges point cooling circuits on the wheel hub mold according to the number of spokes, supporting independent adjustment.
Conclusion and Outlook
Hot spots are not an appearance issue, but a hidden danger to internal quality and machining accuracy.
The linkage of cooling, structure, and rhythm can reduce the temperature of hot spots by up to 25 degrees Celsius.
Extension: Three validations for hot spot treatment
Verification 1: The peak temperature before and after infrared thermal imaging comparison treatment should have a difference of more than 20 degrees Celsius.
Verification 2: Slice inspection of the shrinkage area in the hot spot area should be reduced to below 5%.
Verification 3: The hardness difference measured after machining should be less than 12HB within the same component.
If all three verifications meet the standards, the hot spot treatment can be considered completed.
Just doing some cold work without changing the structure often fails validation two.
Three verification records are archived, and subsequent modifications can directly reuse parameters.
Addendum: Five details of hot spot treatment
The diameter of the cooling pipe at the root of the spoke is often taken as 8 to 10 millimeters, and being too thin can lead to insufficient flow.
The duration of the cold start is set according to the solidification time, usually 5 to 8 seconds after the filling is completed.
The spraying amount in the hot spot area is reduced by about 30%, which can avoid local supercooling and cold insulation.
Adding a transition fillet at the junction of the wheel rim and spokes can reduce the volume of the hot spot by about 20%.
Take one piece from each batch for slicing, and the shrinkage area in the hot spot area should be less than 5%.
Addendum 2: Three acceptance parameters for wheel hub molds
The hardness difference at the root of the spokes should be less than 12HB, exceeding it indicates that the thermal balance has not reached the standard.
The roundness tolerance of the wheel rim is controlled within 0.3 millimeters, and exceeding the tolerance will affect the dynamic balance.
The single piece rhythm is stable within plus or minus 10 seconds, and excessive fluctuations can disrupt the thermal balance.
FAQ
How high is the temperature of the hot spot? Often 30 degrees Celsius higher than the surrounding area.
How low is the hardness of the hot spot area? About 10 to 15HB.
How much temperature can a little cold lower? Locally around 25 degrees Celsius.
What is the required thermal conductivity for inserts? Suggest exceeding 80 watts per meter Kelvin.
What is the size of the rounded corner at the root? Not less than 8 millimeters.
What is the transition length of wall thickness? Take 3 to 5 times the difference in wall thickness.
How to verify hot spots? Infrared thermal imaging with a grid spacing of 50 millimeters.
Gravity casting mold runner design: cross-sectional area ratio and process control
Moldes para fundição por baixa pressão (LPDC)
Moldes para fundição por gravidade
Moldes para fundição por contrapressão (CPC)
Moldes para fundição de peças estruturais
Molde para fundição de cubos de roda de motocicleta
Molde para fundição por pressão diferencial de cubos de roda
Molde para fundição por gravidade de cubos de roda
Molde para fundição por baixa pressão de cubos de roda
MOLDES PARA JANTES AUTOMÓVEIS
PEÇAS ESTRUTURAIS AUTOMÓVEIS
OUTROS COMPONENTES DE FUNDIDOS DE ALUMÍNIO
PERFIL DA EMPRESA
ESTRUTURA ORGANIZACIONAL
HISTÓRICO DE DESENVOLVIMENTO
PROPRIEDADE INTELECTUAL
ESPÍRITO DE EQUIPA PARCEIRO
Copyright © Zhejiang Xinfeng Machinery Co., Ltd. All Rights Reserved.