The key to the release agent is the dosage and concentration. Excessive carbon deposition can worsen both exhaust and heat dissipation.
1、 Concentration to water ratio
Water based release agents are often diluted at a ratio of 1:80 to 1:120, and excessive concentration results in significant residue.
When the concentration exceeds twice the recommended upper limit, the carbon deposition rate accelerates by about twice.
It is recommended to soften the diluted water, as hard water will form white sediment.
2、 Spray quantity and distance
Spray a distance of 200 to 300 millimeters and evenly cover with mist.
Excessive spraying will cause local cooling of the mold cavity, and the temperature difference on the mold surface will increase by about 8 degrees Celsius.
The common distribution principle is to spray less in the thin-walled area and moderate in the hot zone.
3、 Carbon deposition and cleaning
When the thickness of the carbon deposition layer exceeds 0.1 millimeters, the exhaust efficiency decreases by about 30%.
It is recommended to clean the mold every 300 to 500 cycles using a specialized cleaning agent.
When carbon deposits are not cleared, the surface of castings is prone to blemishes, and the repair rate increases.
4、 Relationship with coating
The cavity nitride layer can reduce the demolding resistance by about 15% and reduce the dependence on demolding agents.
The amount of release agent used will increase after coating wear, and it needs to be checked synchronously.
When the coating peels off, the machine should be stopped for treatment to avoid scratching the cavity.
5、 Recording and optimization
Suggest recording the amount of mold release agent and casting demolding situation for each shift.
Abnormal increase in dosage often indicates surface degradation of the cavity.
Industry practice has shown that after standardization of concentration and cleaning, mold defects can be reduced by about 30%.
Conclusion and Outlook
The more release agent, the better. Excessive use can lead to carbon deposition and temperature differences.
Control concentration, distance, and cleaning cycle to reduce both mold sticking and blemishes.
Extension: Three checks for the use of release agents
Check if the dilution ratio is fixed according to the shift, as the mixing error often exceeds 30% based on hand feel.
Check if the spraying trajectory covers the hot zone, and the probability of sticking to the mold at the missed spraying area has significantly increased.
Check if the temperature of the mold cavity is within the spraying window. If it is too low, it may cause liquid accumulation.
Three checks are included in the shift inspection checklist, and complaints about sticking molds usually decrease by about 20%.
The replacement of the release agent brand requires recalibration of the concentration and cannot directly use the old parameters.
The checklist is summarized weekly, and any abnormal trends can be detected in advance.
Addendum: Five detailed rules for on-site management of release agents
It is recommended to control the pressure of the spray gun at 0.3 to 0.5 megapascals. Insufficient atomization when it is too low and wasteful splashing when it is too high.
When the temperature of the mold cavity is below 200 degrees Celsius, spraying is prone to liquid accumulation, and it is necessary to warm it up before spraying.
Record the usage for each shift, and a sudden increase often indicates that the surface of the mold cavity has deteriorated.
Different aluminum liquid grades have different sensitivities to release agents, and recalibration is required when changing grades.
After carbon deposition cleaning, the film layer should be re established, otherwise the first piece is prone to sticking to the mold.
Addendum 2: Three maintenance items for the surface of the mold cavity
Check the mold cavity for scratches every 500 molds, and minor scratches can be treated by polishing.
When the coating wears out and exposes the substrate, it should be redone, otherwise the sticking mold will continue to worsen.
It is recommended to use soft tools for cavity cleaning, as hard scrapers may leave scratches.
Addendum 3: Two principles for selecting release agents
Choose models with lower demolding force for thin-walled parts to reduce protrusion deformation by about 0.5 millimeters.
Choose models that can withstand temperatures above 200 degrees Celsius for high-temperature conditions to avoid film failure.
FAQ
How to dilute the release agent? Regularly press the ratio of 1:80 to 1:120.
What are the consequences of high concentration? The carbon deposition rate is about twice as fast.
What is the spraying distance? 200 to 300 millimeters is more suitable.
How thick is carbon deposition affecting exhaust? If it exceeds 0.1 millimeters, it will decrease by about 30%.
How often should it be cleaned? Suggest every 300 to 500 cycles.
Can hard water be used? Not recommended, it can easily form white sediment.
Can coating reduce release agents? The demolding resistance can be reduced by about 15%.
Maintenance and upkeep of aluminum alloy casting molds: an executable ledger system
Moldes para fundição por baixa pressão (LPDC)
Moldes para fundição por gravidade
Moldes para fundição por contrapressão (CPC)
Moldes para fundição de peças estruturais
Molde para fundição de cubos de roda de motocicleta
Molde para fundição por pressão diferencial de cubos de roda
Molde para fundição por gravidade de cubos de roda
Molde para fundição por baixa pressão de cubos de roda
MOLDES PARA JANTES AUTOMÓVEIS
PEÇAS ESTRUTURAIS AUTOMÓVEIS
OUTROS COMPONENTES DE FUNDIDOS DE ALUMÍNIO
PERFIL DA EMPRESA
ESTRUTURA ORGANIZACIONAL
HISTÓRICO DE DESENVOLVIMENTO
PROPRIEDADE INTELECTUAL
ESPÍRITO DE EQUIPA PARCEIRO
Copyright © Zhejiang Xinfeng Machinery Co., Ltd. All Rights Reserved.