Perguntas frequentes

The difficulty of cylinder head molds lies in the thermal balance of thin-walled water channels, combustion chamber inserts, and multi-point runners.

  • Vistas: ...
  • Tempo de liberação: 2026-11-16

The difficulty of cylinder head molds lies in the thermal balance of thin-walled water channels, combustion chamber inserts, and multi-point runners.

1、 Filling of waterway parts

The wall thickness of the cylinder head water channel is often less than 4 millimeters, and the filling time needs to be controlled between 0.10 and 0.18 seconds.

When the mold temperature in this area is below 280 degrees Celsius, the cold insulation defect rate increases by about 30%.

Local pressure or insulation can increase the filling integrity rate of waterway parts to over 95%.

2、 Thermal management of combustion chamber inserts

The combustion chamber inserts are independently cooled, and the temperature difference between the inlet and outlet water is controlled within 5 degrees Celsius to avoid thermal stress concentration.

The gap between the inlay and the body should be set at 0.05 to 0.08 millimeters, and if it is too large, the aluminum should run out, and if it is too small, it will hold your breath.

The replacement cycle of the insert is usually evaluated based on 20000 to 30000 mold cycles, depending on the depth of the crack.

3、 Multi point gating and sequential solidification

The cylinder head is often poured from 2 to 4 points, and the spacing between the gates is set according to the layout of the air passage to avoid mutual interference.

The solidification sequence should advance from the combustion chamber to the periphery, and reversing the sequence will cause shrinkage and looseness in the nasal bridge area.

Xinfeng simulated the solidification sequence on the cylinder head mold using CAE and adjusted the sprue section ratio to approximately 1:1.8.

4、 Size and sealing

The cylinder head combustion chamber volume tolerance is usually controlled within plus or minus 1.5 milliliters, and exceeding the tolerance affects the compression ratio.

The position tolerance of the valve seat ring hole is taken as 0.15 millimeters, and exceeding the tolerance will cause eccentric wear of the valve.

The flatness of the top surface should be controlled within 0.08 millimeters, otherwise it will cause the cylinder gasket seal to fail.

5、 Validation and Batch Production

The first piece requires CT or slicing, with a focus on examining the nasal bridge area and waterway partition.

One sample is randomly inspected every 200 pieces in batch, and the pressure for air tightness testing is usually taken as 0.15 to 0.2 megapascals.

Industry practice has shown that optimizing the linkage between sprue and insert cooling can reduce the cylinder head scrap rate by about 20%.

Conclusion and Outlook

The success or failure of cylinder head molds lies in thermal balance, rather than single point structural strength.

First, determine the solidification sequence, then set the cooling of the inlay block, and finally calibrate the volume and flatness, significantly reducing the number of repairs.

Extension: Five Quantitative Nodes of the Cylinder Head Project

The wall thickness of the nasal bridge area is often less than 3 millimeters, and the probability of cold insulation increases significantly when the mold temperature is below 280 degrees Celsius.

The temperature difference between the inlet and outlet of the embedded block should be controlled within 5 degrees Celsius, and exceeding it will exacerbate thermal stress.

The gate section ratio is configured at 1:1.8, making sequential solidification easier to achieve.

The combustion chamber volume shall be checked piece by piece, and if the deviation exceeds 1.5 milliliters, the cavity shall be rechecked.

The airtightness test is held for 30 seconds, and if the pressure drop exceeds 5%, it is judged as unqualified.

After quantifying all five nodes, the batch scrap rate of cylinder heads can usually be reduced by about 20%.

Addendum: Three design choices for cylinder head molds

It is recommended to install partial inserts in the nose bridge area, as replacing the inserts alone after damage can save about 60% of repair costs.

When the wall thickness of the waterway partition is less than 3 millimeters, the filling speed needs to be reduced by about 15% to avoid erosion penetration.

When the first piece volume exceeds the tolerance, first check the depth of the nuclear cavity combustion chamber, and then check whether the aluminum liquid shrinkage compensation is calibrated accurately.

FAQ

How thick is the wall of the waterway that needs to be filled quickly? Control within 0.10 to 0.18 seconds when it is below 4 millimeters.

How much is the seam control for inlaid blocks? 0.05 to 0.08 millimeters.

How long does it take to evaluate and replace the inlay? Check the crack depth according to 20000 to 30000 cycles.

What is the tolerance for combustion chamber volume? Usually plus or minus 1.5 milliliters.

Position of valve seat ring? Take 0.15 millimeters.

What is the requirement for top flatness? Control within 0.08 millimeters.

What is the pressure for airtight testing? Usually take 0.15 to 0.2 megapascals.
Intake manifold mold: filling and deformation balance of thin-walled long flow channel

Sítio Web Deste artigo: https://pt.zj-xinfeng.com/case/1475.html

Get a Custom Product Proposal Online

Please fill out the form below to receive this for free.

Global Hotline:

+86-15356852630,13967513266

Moldes para fundição por baixa pressão (LPDC) 
Moldes para fundição por gravidade 
Moldes para fundição por contrapressão (CPC) 
Moldes para fundição de peças estruturais
Molde para fundição de cubos de roda de motocicleta
Molde para fundição por pressão diferencial de cubos de roda
Molde para fundição por gravidade de cubos de roda
Molde para fundição por baixa pressão de cubos de roda

MOLDES PARA JANTES AUTOMÓVEIS 
PEÇAS ESTRUTURAIS AUTOMÓVEIS 
OUTROS COMPONENTES DE FUNDIDOS DE ALUMÍNIO

NOTÍCIAS DA EMPRESA
NOTÍCIAS DO SETOR
BLOG TÉCNICO
PERGUNTAS FREQUENTES

PERFIL DA EMPRESA
ESTRUTURA ORGANIZACIONAL
HISTÓRICO DE DESENVOLVIMENTO
PROPRIEDADE INTELECTUAL
ESPÍRITO DE EQUIPA PARCEIRO

Copyright © Zhejiang Xinfeng Machinery Co., Ltd. All Rights Reserved.