Perguntas frequentes

The shell mold cavity is deep and has many ribs, and 70% of the defects come from poor exhaust and incomplete cleaning of residual aluminum.

  • Vistas: ...
  • Tempo de liberação: 2026-11-16

The shell mold cavity is deep and has many ribs, and 70% of the defects come from poor exhaust and incomplete cleaning of residual aluminum.

1、 Layered arrangement of exhaust system

The exhaust parting groove, insert slot, and top needle gap of the gearbox housing casting mold are arranged in three layers.

The distance between the exhaust grooves in the deep cavity area of the mold is set to 25 to 30 millimeters, and the distance in the final filling area is increased to 15 millimeters.

When the total exhaust area is insufficient, the porosity of the housing cavity will increase to over 4%.

2、 Inlaid blocks and seams

Deep cavity parts are often assembled with embedded blocks, and the gap between the joints is controlled at 0.05 to 0.10 millimeters.

If the seam is too large, aluminum will run away, and if it is too small, gas cannot be discharged. Both situations will increase the scrap rate.

The independent water flow of the embedded block cooling can reduce the mold temperature in the deep cavity area by about 20 degrees Celsius.

3、 Residual aluminum and cleaning

The shell mold needs to be cleaned every time it stops, and residual aluminum thickness exceeding 0.1 millimeters will affect the next filling.

The recommended cleaning cycle is once every 20 molds, using dry ice or specialized cleaning agents.

Xinfeng has reserved cleaning channels and exhaust detection points on the shell mold for easy maintenance of the production line.

4、 Size and sealing surface

The flatness of the joint surface between the shell and the end cap is usually controlled within 0.1 millimeters, otherwise oil leakage may occur.

The tolerance for the roundness of the bearing hole is set at 0.05 millimeters. Exceeding this tolerance will result in abnormal noise and wear.

Thermal deformation of the mold cavity can cause flatness drift, which needs to be compensated according to the measured mold temperature.

5、 Batch and Foreign Trade

A single set of shell molds often has 2 to 4 cavities, and the consistency tolerance of multiple cavities needs to be controlled within 0.15 millimeters.

European customers generally require airtightness test reports, and sealing verification must be done during the trial molding stage.

Industry data shows that after exhaust optimization, the repair rate of shell air holes can be reduced by about 30%.

Conclusion and Outlook

The bottleneck of production capacity for shell molds often lies in cavity cleaning and exhaust, rather than in machine tools.

The inclusion of exhaust stratification, insert gap, and cleaning cycle in the mold specifications has significantly improved stability.

Extension: Key points for purchasing complex shell molds

Request the supplier to provide a cavity layout diagram, as insufficient cavity spacing will limit the cooling layout.

Check the number of inserts and disassembly methods. Excessive inserts can prolong a single maintenance by about two hours.

Confirm whether the cleaning channel and detection point are reserved, as missing them may result in shutdown for processing.

Confirm that the tonnage of the press matches the weight of the mold. Overloading will limit the closing speed of the mold.

Confirm that the accompanying documents contain records of air tightness testing. Any missing records need to be supplemented and delayed for acceptance.

Include the key points in the inquiry form, improve the comparability of quotations, and shorten the review time by about 30%.

Addendum: Three maintenance experiences for shell molds

It is recommended to perform independent ejection for deep cavity inserts, as uneven force during overall ejection can cause the insert to shift by about 0.1 millimeters.

The diameter of dry ice particles used for cleaning the cavity should be 3 millimeters. If it is too large, it can easily damage the surface of the cavity and the exhaust slot.

When the airtightness test fails, check the flatness of the joint surface first, and then check the internal porosity. The order cannot be reversed.

FAQ

What is the spacing between exhaust ducts? The deep cavity area is 25 to 30 millimeters, and the final filling area is 15 millimeters.

How much is the seam control for inlaid blocks? 0.05 to 0.10 millimeters, if the aluminum is too large or too small, hold your breath.

How long is the cavity cleaning cycle? It is recommended to do it every 20 times.

How thick is the residual aluminum that needs to be cleaned? Exceeding 0.1 millimeters affects the filling process.

What is the flatness of the joint surface? Usually controlled within 0.1 millimeters.

What is the tolerance for bearing hole roundness? Take 0.05 millimeters, there will be abnormal noise if it exceeds the tolerance.

Consistency requirements for multiple cavities? The tolerance is controlled within 0.15 millimeters.

Cylinder head mold: process difficulties in the waterway and combustion chamber parts

Sítio Web Deste artigo: https://pt.zj-xinfeng.com/case/1474.html

Get a Custom Product Proposal Online

Please fill out the form below to receive this for free.

Global Hotline:

+86-15356852630,13967513266

Moldes para fundição por baixa pressão (LPDC) 
Moldes para fundição por gravidade 
Moldes para fundição por contrapressão (CPC) 
Moldes para fundição de peças estruturais
Molde para fundição de cubos de roda de motocicleta
Molde para fundição por pressão diferencial de cubos de roda
Molde para fundição por gravidade de cubos de roda
Molde para fundição por baixa pressão de cubos de roda

MOLDES PARA JANTES AUTOMÓVEIS 
PEÇAS ESTRUTURAIS AUTOMÓVEIS 
OUTROS COMPONENTES DE FUNDIDOS DE ALUMÍNIO

NOTÍCIAS DA EMPRESA
NOTÍCIAS DO SETOR
BLOG TÉCNICO
PERGUNTAS FREQUENTES

PERFIL DA EMPRESA
ESTRUTURA ORGANIZACIONAL
HISTÓRICO DE DESENVOLVIMENTO
PROPRIEDADE INTELECTUAL
ESPÍRITO DE EQUIPA PARCEIRO

Copyright © Zhejiang Xinfeng Machinery Co., Ltd. All Rights Reserved.