Shrinkage and porosity of gravity casting molds: three quantifiable strategies

Seventy percent of the shrinkage and porosity in gravity castings are caused by mismatches in three parameters: sprue, exhaust, and mold temperature.

1、 The proportion of the pouring channel should be addressed first to compensate for shrinkage

The area ratio of the sprue and runner in gravity casting molds is often taken as 1:1.6 to 1:2.0.

A too small cross-sectional area of the sprue will result in insufficient compression pressure and an increase of about 8 percentage points in the failure rate of shrinkage.

By widening the sprue by 10% and using the top riser, the shrinkage and looseness in the thick walled area can be reduced to within 3%.

2、 The position of the exhaust groove is more important than the quantity

The total cross-sectional area of the exhaust groove shall be configured to be no less than 8 square millimeters per 100 square centimeters of the projected area of the cavity.

The exhaust groove is located in the final filling area of the aluminum liquid, and the porosity can be reduced by about 40%; Opening the wrong position is almost ineffective.

The groove depth should be controlled between 0.2 and 0.3 millimeters. If it is too deep, aluminum will run away, and if it is too shallow, exhaust will not be smooth.

3、 Mold temperature zoning control to restrain shrinkage porosity

The mold temperature for thin-walled areas is set at 280 to 320 degrees Celsius, while for thick walled areas it is set at 350 to 380 degrees Celsius, forming a sequential solidification process.

When the mold temperature is below 250 degrees Celsius, the probability of cold insulation defects increases by about 30%.

Xinfeng's gravity casting mold is equipped with independent thermocouples near the sprue and riser, and the mold temperature fluctuation is controlled at plus or minus 8 degrees Celsius.

4、 Coatings and Aluminum Liquid Treatment

Coating layer thickness exceeding 0.15 millimeters can hinder heat dissipation, leading to local overheating and mold sticking.

After refining the aluminum liquid, the gas content should be controlled below 0.15 milliliters per 100 grams, and the porosity can be reduced by about 35%.

For every 10 degrees Celsius increase in pouring temperature, the suction volume increases by about 12%, and the lower limit should be set for thin-walled parts.

5、 Verification method and judgment

The first piece should be inspected by X-ray or slicing, and the proportion of shrinkage area should be less than 5% before entering the batch.

During the batch stage, one piece will be sampled every 200 pieces, and if three consecutive batches pass, the sampling frequency will be relaxed.

Industry data shows that the joint optimization of sprue and exhaust can increase the yield of gravity castings by about 15 percentage points.

Conclusion and Outlook

Shrinkage and porosity are not the same problem. Shrinkage relies on filling, while porosity relies on exhaust and degassing, and cannot be treated interchangeably.

First confirm the solidification sequence with CAE, then determine the runner and exhaust, and the number of mold tests can usually be saved once.

Extension: Six parameters often overlooked on site

When the moisture content of the sand core is higher than 0.3%, the porosity will significantly increase, and the drying time needs to be correspondingly extended.

When the liquid level drop of the pouring cup exceeds 50 millimeters, the amount of gas entrapment increases and the proportion of inclusions and defects increases.

Insufficient preheating of the mold results in a 20% higher probability of cold insulation for the first piece compared to subsequent pieces, wasting one opportunity for mold testing.

The size of the riser is determined based on experience, and insufficient shrinkage will result in a shrinkage area of more than 5% in the thick walled area.

Using the same set of parameters to produce parts with different wall thicknesses can result in a defect rate fluctuation of up to 10 percentage points.

By setting the pouring speed and mold temperature according to the wall thickness, the yield improvement is usually over 10%, and the repair time decreases synchronously.

FAQ

What is the ratio of the area of the sprue to the area of the runner? Commonly used ratios range from 1:1.6 to 1:2.0.

What is the appropriate depth for the exhaust groove? 0.2 to 0.3 millimeters, fine tuned according to the casting wall thickness.

How low is the mold temperature that is prone to cold insulation? The probability of temperatures below 250 degrees Celsius has significantly increased.

How much gas content should be controlled in aluminum liquid? Less than 0.15 milliliters per 100 grams.

What is the qualified line for shrinkage area? If the first piece ratio is less than 5%, it can enter the batch.

Is it better to pour at a higher temperature? No, the air intake increases by about 12% per liter at 10 degrees Celsius.

What is the appropriate thickness for the coating layer? Not exceeding 0.15 millimeters, excessive thickness will stick to the mold.

Sítio Web Deste artigo: https://pt.zj-xinfeng.com/case/1469.html

Get a Custom Product Proposal Online

Please fill out the form below to receive this for free.

Global Hotline:

+86-15356852630,13967513266

Moldes para fundição por baixa pressão (LPDC) 
Moldes para fundição por gravidade 
Moldes para fundição por contrapressão (CPC) 
Moldes para fundição de peças estruturais
Molde para fundição de cubos de roda de motocicleta
Molde para fundição por pressão diferencial de cubos de roda
Molde para fundição por gravidade de cubos de roda
Molde para fundição por baixa pressão de cubos de roda

MOLDES PARA JANTES AUTOMÓVEIS 
PEÇAS ESTRUTURAIS AUTOMÓVEIS 
OUTROS COMPONENTES DE FUNDIDOS DE ALUMÍNIO

NOTÍCIAS DA EMPRESA
NOTÍCIAS DO SETOR
BLOG TÉCNICO
PERGUNTAS FREQUENTES

PERFIL DA EMPRESA
ESTRUTURA ORGANIZACIONAL
HISTÓRICO DE DESENVOLVIMENTO
PROPRIEDADE INTELECTUAL
ESPÍRITO DE EQUIPA PARCEIRO

Copyright © Zhejiang Xinfeng Machinery Co., Ltd. All Rights Reserved.